En10025-5 S355K2W Kimyoviy tarkibi

 

Baho

Kimyoviy tarkibi

S355K2W

Element maksimal (%)

C

Si

Mn

P

S

N

Kri

Ku

0.19

0.55

0.45-1.60

0.035

0.035

-

0.35-0.85

0.20-0.60

 

En10025-5 s355k2w mexanik mulk

 

rada

Mexanik mulk

S355K2W

Kuch berish kuchi
mm
Min (MPA)

Mustahkamlik chegarasi
mm
Min (MPA)

 

Elegyonmin,%

 

16 dan kam yoki teng

>16
Dan kam yoki unga teng
40

>40
Dan kam yoki unga teng
63

>63
Dan kam yoki unga teng
80

>80
Dan kam yoki unga teng
100

>100
Dan kam yoki unga teng
150

<3

Dan katta yoki teng
3
Dan kam yoki unga teng
100

Dan katta yoki teng
100
Dan kam yoki unga teng
150


1.5
Dan kam yoki unga teng
2


2
Dan kam yoki unga teng
2.5

>2.5

3

>3
Dan kam yoki unga teng
40

>40
Dan kam yoki unga teng
63

>63
Dan kam yoki unga teng
100

>100
Dan kam yoki unga teng
150

355

345

335

325

315

295

510-680

470-630

450-600

14

15

16

20

19

18

18

 

S355K2W Issiqlik bilan ishlash: issiq rulonli, normallashtirilgan, normallangan, qonli va temperli sovuq.

 

S355K2W po'lat plastinkako'prik va kuchaytirilgan korroziyalarga chidamliligi talab qilinadigan ko'priklar va boshqa tuzilmalarning qurilishi, mahkamlangan yoki boshqa tuzilmalarni qurish uchun mo'ljallangan.

 

Gnee po'lat - bu strukturaviy po'lat plastinka va palanlarning tarkibiy atmosfera korroziyalariga chidamlidir. Bizning omborxonasida 10000 tonna po'lat plitasi va ob-havoga chidamli po'lat plastinkaga bo'yalgan.

 

Shunday qilib, biz etkazib berish vaqtini va raqobatbardosh narxni boshqa kompaniya bilan taqqoslashiga va'da beramiz.

 

S355K2W narxini olish uchun hozir bilan bog'laning

 

info-834-452